Why filler-wire-only welding requires closer scrutiny in safety-critical AlSi-coated PHS applications
In safety-critical PHS applications, a continuous weld or one acceptable test result does not prove that the process is robust. Robustness means maintaining controlled chemistry, microstructure, mechanical behaviour, and performance as coating weight, sheet thickness, material combinations, and production conditions vary.
</Article 5> set out the evidence every safety-critical weld seam must provide. This article applies that standard to filler-wire-only welding, where enriched wire is used to compensate for aluminium after the AlSi coating has entered the weld pool.
In a filler-wire-only (FWO) process, the AlSi coating remains on the welding edge and aluminium enters the molten weld pool. Enriched filler wire introduces alloying elements intended to counteract its metallurgical effects.
The amount of aluminium entering the weld varies with sheet thickness, coating weight, material pairing, seam configuration, and normal production tolerances. The required level of compensation therefore changes with the welding condition.
Maintaining the correct balance would require wire input to adapt continuously to coating variation. Current feedback control cannot respond at the speed required to measure and correct that variation during welding. A fixed wire input may therefore undercompensate in one condition and overcompensate in another.
Using excess wire to cover the uncertainty creates further process risks, including unstable welding and convex or irregular seam geometry.
FWO compensates for aluminium only after a variable amount has already entered the weld pool. Partial ablation takes a different approach by reducing that variation before welding.
Average aluminium content does not show how aluminium is distributed through the weld. In FWO welding, uneven mixing can leave aluminium-rich zones within a seam whose overall chemistry appears acceptable.
These zones can develop a different microstructure from the surrounding weld. At higher aluminium concentrations, coarse delta-ferrite may remain after hot stamping, reducing hardness and ductility and creating a local region where fracture can initiate.
In one FWO example assessed by ArcelorMittal, the weld showed an average aluminium content of approximately 1.1 wt%, while a local zone reached 4.5 wt%. The average appeared close to the identified limit but concealed a much more severe local condition.
As vehicle architectures evolved further, a single PHS grade could no longer meet all structural and crash requirements within one component.
Different zones of the same part must perform different functions. Some areas need maximum resistance to intrusion, while others must absorb energy through controlled deformation. Achieving both within a single structure requires more than uniform material properties.
To meet this need, the material portfolio expanded to support functional differentiation. Usibor® 1500 became the reference for high-strength anti-intrusion zones, while Ductibor® 450 and 500 provide higher ductility for energy absorption. This approach was extended with Ductibor® 1000, which combines strength and ductility for more demanding crash scenarios, and Usibor® 2000, which supports further weight reduction at very high strength levels. More recent developments, such as Ductibor® 1500, continue to extend the available design options.
This evolution allows engineers to define local behaviour within a single component, placing strength and ductility where they are needed instead of using uniform material properties.

Average aluminium content can conceal the local conditions that control weld behaviour. Even when the overall value remains near the identified limit, uneven mixing may create aluminium-rich zones that reduce quenchability, alter microstructure, and increase the risk of brittle fracture.
Technical analysis identifies approximately 1.2 wt% aluminium as an important upper boundary for delta-ferrite formation under the conditions assessed. Remaining below that average does not demonstrate homogeneous mixing, uniform microstructure, or repeatable weld behaviour. Aluminium at lower levels can still affect austenitisation, quenchability, and hardness after hot stamping.
Average chemistry must therefore be supported by local measurements. Without them, the condition that controls fracture behaviour may remain hidden.
An examination of one production door ring shows why weld robustness cannot be judged from average chemistry or nominal tensile strength alone.
The component showed no evidence of coating ablation. Samples from the weld revealed heterogeneous mixing, reduced microhardness, irregular seam geometry, variation between tensile results, and fracture within the weld.
Together, these findings point to inconsistency within the same component. Local chemistry varied, hardness was reduced, geometry was uneven, and mechanical performance changed between tests. Fracture within the weld also shows that the seam became the controlling region under the conditions examined.
This case does not obviously represent every FWO application. But it does show why a single average value or passing result cannot establish process robustness.
Robustness requires consistency across chemistry, hardness, geometry, tensile behaviour, and failure location. Where those characteristics vary within one production component, the process window needs closer scrutiny.
The preceding evidence points to a practical requirement: assessment has to extend beyond a passing result and consider how the process behaves across the full production window. Three questions help focus that review.
The relevant figure is not the nominal aluminium level for one material combination. The assessment should show how aluminium input changes with coating weight, sheet gauge, and mixed-thickness configurations.
It should also show how FWO input is adjusted as those conditions change, and whether testing covers worst-case combinations as well as nominal ones.
Average chemistry is not sufficient. Local measurements should show how aluminium is distributed through the depth of the seam, whether mixing remains consistent, and whether aluminium-rich zones are present.
The resulting microstructure and hardness should also remain uniform across the weld.
Repeatability should be demonstrated through weld geometry, hardness profiles, tensile scatter, and failure location.
That evidence should cover multiple coating weights, steel-grade pairings, and thickness combinations, rather than one optimised sample.
These questions do not assume that FWO will fail. They simply establish whether the process has demonstrated a robust production window.
FWO can alter weld chemistry, but its presence alone does not demonstrate control across the full production window. That requires local measurements showing that aluminium distribution, microstructure, hardness, and mechanical behaviour remain consistent across material combinations and production variation.
Repeatability under static testing is still not the final proof. A safety-critical seam must also be validated under the loading conditions it is expected to experience in a crash.
The next article examines why a favourable static result may still leave a critical evidence gap, and how dynamic impact testing reveals the difference between ductile weld behaviour and brittle fracture.